Stainless Steel 422 (AMS 5655)
Technical Data Sheet
Chemical Composition Limits | ||||||||||||
Weight% | C | P | Si | Ni | V | Fe | Mn | S | Cr | Mo | W | Cu |
Alloy 422 | 0.20-0.25 | 0.040 max | 0.20-0.60 | 0.50-1.0 | 0.17-0.30 | Bal | 1.0 | 0.030 max | 11.0-13.5 | 0.75-1.25 | 0.75-1.25 | 0.50 |
Alloy 422 is a hardenable stainless steel designed for use at temperatures of up to 1200ºF (649ºC). Alloy 422 has good resistance to scaling and oxidation. Through heat treatment, high mechanical properties can be developed. Alloy 422 is used in applications such as compressors or steam turbines and also in aircraft parts, valves, high temperature bolting etc.
Typical Mechanical Properties
Material | Condition | 0.2 % Yield Strength (ksi) | Ultimate Tensile Strength (ksi) | % Elongation in 2" | % Reduction of Area | Hardness HB |
Alloy 422 | Hardened & Tempered (AMS 5655) | 140 | 115 | 13 | 25 | 293-341 |
Availability
Alloy 422 is available as Bar (Round, Shapes), Billet, Wire, Strip, Flat Bar, Forgings.
Specifications
UNS S42200
AISI 616
AMS 5655 Bars / wire/ forging H&T
ASTM A 565 GRD 616
DOD F 24669/7
MIL S 861
B50A125 (Cap of)
B50A951A1 (Cap of)
BS 970; 442S19
EN61